Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3ZG6 BK20591 - PA66-I-GF30 - BASF

Material Data Center offers the following functions for Ultramid® A3ZG6 BK20591:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
An impact-modified, glassfibre reinforced injection moulding grade with good dimensional stability.
Caracteristicas de procesamiento y fisicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 15 / * cm³/10min ISO 1133
Temperatura 275 / * °C -
Carga 5 / * kg -
Contracción posterior al moldeo, paralelo 0.5 / * % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0.9 / * % ISO 294-4, 2577
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 8500 / 6000 MPa ISO 527
Resistencia a la tracción 140 / 100 MPa ISO 527
Alargamiento a rotura 3.5 / 6 % ISO 527
Módulo de plastodeformación, 1000h * / 3000 MPa ISO 899-1
Resistencia al impacto Charpy, +23°C 90 / 95 kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C 85 / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 19 / 26 kJ/m² ISO 179/1eA
Resistencia al impacto Charpy c/entalla, -30°C 10 / - kJ/m² ISO 179/1eA
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 260 / * °C ISO 11357-1/-3
Estabilidad al calor, 1.80 MPa 240 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 250 / * °C ISO 75-1/-2
Coef.de expansión térmica lineal, paralelo 27 / * E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 128 / * E-6/K ISO 11359-1/-2
Combustibilidad a 1.5mm esp. nom. HB / * class IEC 60695-11-10
Espesores de probeta 1.6 / * mm -
Yellow Card disponible sí / * - -
Combustibilidad a espesor h HB / * class IEC 60695-11-10
Espesores de probeta 0.8 / * mm -
Yellow Card disponible sí / * - -
Ratio de combustión, FMVSS, Espesor de 1mm 0 mm/min ISO 3795 (FMVSS 302)
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Constante dieléctrica, 1MHz 3.5 / 5.5 - IEC 62631-2-1
Factor de pérdidas dieléctricas, 1MHz 140 / 1600 E-4 IEC 62631-2-1
Resistividad volumétrica específica 1E13 / 1E10 Ohm*m IEC 62631-3-1
Resistividad superficial específica * / 1E10 Ohm IEC 62631-3-2
Indice comparativo de linea de fuga - / 550 - IEC 60112
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 5 / * % Sim. to ISO 62
Absorción de humedad 1.5 / * % Sim. to ISO 62
Densidad 1330 / - kg/m³ ISO 1183
Propiedades específicas del materialSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de viscosidad 160 / * cm³/g ISO 307, 1157, 1628
Condiciones de transformaciónValorUnidadesMétodo de ensayo
ISO Data
Moldeo por inyección, temperatura de la masa 290 °C ISO 294
Moldeo por inyección, temperatura del molde 80 °C ISO 294
Moldeo por inyección, velocidad de inyección 200 mm/s ISO 294
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 80 °C -
Tiempo de pre-secado 4 h -
Humedad de procesamiento ≤0.15 % -
Temperatura de la masa 280 - 300 °C -
Temperatura del molde 80 - 90 °C -
Funciones
Viscosidad-velocidad de cizallamiento , Ultramid® A3ZG6 BK20591, PA66-I-GF30, BASF
Tensión de cizalla-velocidad de cizalla , Ultramid® A3ZG6 BK20591, PA66-I-GF30, BASF
Módulo de cizallamiento dinámico-temperatura , Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo de cizallamiento dinámico-temperatura , Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Esfuerzo-alargamiento , Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Esfuerzo-alargamiento , Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Módulo secante-alargamiento , Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo secante-alargamiento , Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Esfuerzo-alargamiento (isocrono) 23°C, Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Módulo de plastodeformación-tiempo 23°C, Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Curva de creep 23°C, Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Esfuerzo-alargamiento (isocrono) 80°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo de plastodeformación-tiempo 80°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Curva de creep 80°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Esfuerzo-alargamiento (isocrono) 120°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo de plastodeformación-tiempo 120°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Curva de creep 120°C, Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo a tensión-temperatura , Ultramid® A3ZG6 BK20591 (Seco), PA66-I-GF30, BASF
Módulo a tensión-temperatura , Ultramid® A3ZG6 BK20591 (Cond), PA66-I-GF30, BASF
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Sémola, Negro
Aditivos
Lubricante, Desmoldeante
Características especiales
Alto impacto o modificado al impacto, Estable contra el calor
Disponibilidad regional
Demás información
Moldeo por inyección
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com